?Objective: To evaluate the mechanical properties of low noble alloy Au Pd and Ag Pd developed by Stomatological College,Fourth Millitaly Medical University and Xi'an University of Architecture & Techuology. Methods:The two low noble alloys were cast by means of a centrifugal induction furnace into the tensile bars whose dimensions accorded with the standards of China for Dental Casting Precious Metal Alloys. Tensile properties (?b)were determined by means of a conventional testing machine. The 0.2% offset yield strength(?0.2), elongation(?) and microhardness (HV)were determined in a conventional manner. All data were the average of four specimens of each alloy. Results:?b(MPa),?0.2(MPa),?(%) and HV of Au Pd were 485?12.9,365 ?14.8,7.8?1.1 and 220?14.3;those of Ag Pd 550?9.5,435?8.2,13.5?5.4 and 245?15.1,respectivey.Conclusion:The mechanical properties of the two low noble alloys meet the demands of standards and have lower microhardness than natural tooth enamel.